Abstract |
Fe solubility in AZ91 alloy melts was measured by a new method designed for removal of Al_(8)(Mn,Fe)_(5) inclusions. In the AZ91 alloy melts, Al_(8)(Mn,Fe)_(5) precipitates were formed due to supersaturated Mn and Fe, but all precipitates were not settled down from the melts and hence part of them was included in the samples for measuring Fe solubility. This means that the solubility measured from these samples is higher than the true solubility. In the present study, it was shown that these Al_(8)(Mn,Fe)_(5) inclusions could be separated from the samples by the new method. As a result, the Fe solubility measured by the present method was lower than the previous solubility data. Amount of the unsettled Al_(8)(Mn,Fe)_(5) inclusions was estimated to be 59-148 ppm. It was also observed that Fe contents in Al_(8)(Mn,Fe)_(5) were varied with the Fe and Mn content in AZ91 alloy melts. |
|
|
Key Words |
Fe solubility, AZ91 alloy, Magnesium, Precipitate, Inclusion |
|
|
 |
|